Remove visible oversized material prior to compacting
Appearance of Uncoated Material in CCPR Mix
Adjust recycling agent and water to compensate
Mix Segregation
If by mechanical separation, check RAP loading in cold feed hoppers, buildup and/or worn paddles in the pugmill, and screed transfer augers of the paver
If inadequate asphalt coating of the aggregate due to inadequate water content or recycling agent, adjust application rates
Varying Dry and Wet Spots in RAP
Check water and/or recycling agent application systems.
Adjust application rates if caused by RAP gradation changes
Oversize or Undersized RAP in Mix
Check screening/crushing unit or scalping screen
Flushing of Asphalt at Surface
If excessive mix water, reduce the target water content in the mix
If excessive recycling agent, reduce asphalt content
If Inadequate mixing of materials, check mixing chamber for signs of wear/build up
Mat Stays Spongy and/or Will Not Densify
Reestablish control strip and/or density rolling pattern
If steel wheel rollers are sealing the surface and causing moisture retention, use a heavy pneumatic tire roller for the breakdown and compaction rolling
If excess moisture is in the mix, revise recycling agent and water as necessary
Post-Construction Troubleshooting
Dimpled CR mix due to parked traffic on fresh mat
Dimpling Due to Parked Vehicles or Equipment
Tack and fill with asphalt mixture (cold mix, recycled mix, WMA or HMA) prior to placing surface course
Permanent Deformation
Within Wheel Path Areas Due to Secondary Compaction by Traffic: If pavement temperatures permit, apply secondary compaction. Tack and fill with asphalt mixture (cold mix, recycled mix, WMA, or HMA) or micro surfacing in the low areas or cold mill to provide a smooth surface
Permanent Deformation and Shoving Due to Unstable Mix: Investigate pavement structure in conjunction with mix design lab. Depending on investigation, remove tack and replace affected areas with asphalt mixture (cold mix, recycled mix, WMA, or HMA) or re-recycle supplementing with uncoated coarse aggregate, additives and/or recycling agent as necessary
Raveling, Scuffing or Tearing
Isolated Areas of Minor Raveling or Scuffing: Sweep and monitor. Determine if fog sealing or re-fog sealing is necessary to protect
Isolated Areas of Major Raveling, Scuffing or Tearing: Maintain better traffic restrictions in areas that are not cured. Sweep and monitor. Determine if fog sealing or re-fog sealing is necessary to protect. Tack and fill or remove tack and replace deep damaged areas with asphalt mixture (cold mix, recycled mix, WMA, or HMA) prior to surface course
Large Scale Areas of Raveling, Scuffing or Tearing in Straight Traffic Areas: Re-recycle or remove tack and replace with asphalt mixture (cold mix, recycled mix, WMA, or HMA)
High Spots out of Surface Tolerance
Correct humps exceeding tolerance by reworking, rerolling, trimming or milling and fog seal as necessary
Let's Connect
Get the latest in industry trends, research, success stories, and technical updates in a succinct e-newsletter.
PPRA Industry News Signup
Thank you!
Thank you for signing up for the PPRA mailing list!
If you created an account, you should receive an email shortly with more instructions to activate your account.